| 3.7 | 3.93 | 3.92 | 3.96 | |||
| Crystal , Avg | MICRONS | THIN-SECTION | 12 | 6 | 6 | 3 |
| White | Ivory | Ivory | Ivory | |||
| Flexural Strength (MOR), 20 degree |
MPa | ASTM-F417 | 352 (51) | 400 (58) | 375 (54) | 552 (80) |
20 degrees |
303 (44) | 370 (54) | 370 (54) | 386 (56) | ||
|
Poisson's Ratio 20 degrees |
* | ASTM-C848 | 0.21 | 0.22 | 0.22 | 0.24 |
20 degrees |
2103 (305) | 2680 (390) | 2500 (363) | 3792 (550) | ||
|
Fracture Toughness, Klc |
Mpa m^1/2 | Notched Beam | 4 5 | 4 5 | 4 5 | 4 5 |
20 degree |
22.4 | 30 | 30 | 36 | ||
| CTE, 25-1000 degrees | 1X10^-6/ C | ASTM-C372 | 8.2 | 8.2 | 8.2 | 8.4 |
Resistance |
250 | 200 | 200 | 200 | ||
| Maximum Use Temp. | C | NO-LOAD COND. | 1700 | 1750 | 1750 | 1900 |
25 Degrees |
>10^14 | >10^14 | >10^14 | >10^14 | ||
|
Volume Resistivity, 500 Degrees |
Ohm-cm | ASTM-D1829 | 4 X 10^9 | 1 X 10^10 | 2 X 10^10 | 3.3 X 10^12 |
1000 Degrees |
5 X 10^5 | 3 X 10^6 | 2 X 10^6 | 1.1 X 10^7 | ||
| Hardness | GPa | Rockwell 45N | 78 | 83 | 83 | 90 |